Hot Cracking in Stainless Steel Welds: Causes, Detection, and Prevention

Jun 23, 2026

Leave a message

Emily Li
Emily Li
Quality Control Manager at Jinie Technology, dedicated to ensuring the highest standards in stainless steel and alloy production. Skilled in ISO compliance, material testing, and process improvement. A advocate for precision and excellence.

Hot cracking-also known as solidification cracking-is the most common welding defect in stainless steel fabrication, accounting for approximately 60-70% of all weld failures in austenitic stainless steels. This phenomenon occurs when liquid films or low-melting phases become trapped at grain boundaries during solidification, creating weak paths that cannot withstand the thermal contraction stresses of cooling. The fundamental cause is excessive impurity segregation (sulfur, phosphorus, silicon) combined with inappropriate weld geometry or excessive heat input.

 

Cracking in Stainless Steel Welds

 

This article presents a comprehensive, evidence-based analysis of hot cracking mechanisms, detection methods, and prevention strategies across five major stainless steel families.

 

What is Hot Cracking?

 

Hot cracking occurs during the final stages of weld solidification when the metal is partially liquid and partially solid. Imagine chocolate that's halfway between melted and solid-it's weak and can easily split apart. Similarly, stainless steel at this stage has weak grain boundaries because low-melting impurities (like sulfur and phosphorus) get pushed to the edges of growing crystals. When the weld cools and shrinks, these weak boundaries crack open. The cracks typically appear within 0.1-10 mm of the weld centerline and can be microscopic or visible to the naked eye.

 

The Three Types of Hot Cracking

 

Solidification cracking: Occurs during initial welding as the molten pool solidifies (most common, 80% of cases)

 

Liquation cracking: Occurs in the heat-affected zone (HAZ) when existing grains partially melt during welding

 

Ductility-dip cracking: Occurs at 800-1000°C when the metal loses ductility due to precipitation of brittle phases

 

Solidification cracking is the primary focus of this article because it accounts for the vast majority of field failures and is directly influenced by weld procedure variables that fabricators can control.

 

Sulfur and Phosphorus Are the Primary Culprits

 

Direct Evidence: Sulfur (S) and phosphorus (P) are the two most harmful impurities that cause hot cracking in stainless steel welds. When present above 0.015% (150 ppm) for sulfur or 0.020% (200 ppm) for phosphorus, these elements form low-melting compounds that remain liquid after the surrounding metal has solidified. The sulfur compound (manganese sulfide, MnS) melts at 1,615°C, but when combined with iron and chromium, the melting point drops to 950-1,050°C-well below the 1,400-1,450°C solidification temperature of stainless steel. This creates liquid films at grain boundaries that cannot withstand shrinkage stresses.

 

Table. Sulfur and Phosphorus Content Limits for Hot-Crack-Resistant Stainless Steels

 

         

Material Grade

Max S (‰)

Max P (‰)

Typical Crack Susceptibility

Standard

304/304L (standard)

0.030

0.045

High

ASTM A240

304L (L-grade, low C)

0.030

0.045

Moderate-High

ASTM A240

316/316L (standard)

0.030

0.045

High

ASTM A240

321 (Ti-stabilized)

0.030

0.045

Moderate

ASTM A240

347 (Nb-stabilized)

0.030

0.045

Moderate

ASTM A240

904L (high alloy)

0.020

0.030

Low-Moderate

ASTM B625

254 SMO (6% Mo)

0.010

0.030

Low

UNS S31254

AL-6XN (super austenitic)

0.010

0.020

Very Low

UNS N08367

Welding filler (ER308L)

0.020

0.030

Low (proper filler)

AWS A5.9

Welding filler (ER316L)

0.020

0.030

Low (proper filler)

AWS A5.9

Source: ASTM A240/A240M-22 'Standard Specification for Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip'; AWS A5.9/A5.9M-22 'Specification for Bare Stainless Steel Welding Electrodes and Rods'; IIW (International Institute of Welding) Document IX-2202-18 'Guidelines for the Prevention of Hot Cracking in Austenitic Stainless Steel Welds.'

 

Key Takeaway: Simply using 'L-grade' steel (low carbon, ≤ 0.030% C) does NOT guarantee hot-crack resistance. The critical impurities are sulfur and phosphorus, not carbon. Low-carbon grades reduce sensitization risk but have minimal effect on solidification cracking. For crack-resistant welds, specify steel with S ≤ 0.015% and P ≤ 0.020%.

 

Austenitic Stainless Steels Are Most Susceptible

 

Austenitic stainless steels (300-series: 304, 316, 321, 347) are 5-10 times more susceptible to hot cracking than ferritic or duplex stainless steels. This is because austenitic (face-centered cubic, FCC) crystals have more impurity solubility than ferritic (body-centered cubic, BCC) crystals, allowing more sulfur and phosphorus to segregate to grain boundaries during solidification. Duplex steels (22% Cr, 5% Ni, 3% Mo) have a mixed austenite-ferrite structure that interrupts the continuous liquid films, reducing cracking susceptibility by 70-80% compared to fully austenitic steels.

 

Austenitic Stainless Steels Are Most Susceptible

 

Table. Hot Cracking Susceptibility by Stainless Steel Family

 

           

Steel Family

Typical Grades

Crystal Structure

Relative Crack Susceptibility

Ferrite in Weld (FN)

Prevention Difficulty

Austenitic (most susceptible)

304, 316, 321, 347

100% FCC (austenite)

100% (baseline)

0-5 FN (prone)

Difficult

Austenitic (L-grade)

304L, 316L

100% FCC

80% (slightly better)

0-5 FN

Moderate-Difficult

Austenitic (high-purity)

904L, AL-6XN

100% FCC (low S/P)

40% (much better)

0-3 FN

Moderate

Duplex (least susceptible)

2205 (S31803)

50% FCC + 50% BCC

20% (low risk)

40-60 FN (ideal)

Easy

Super Duplex

2507 (S32750)

50% FCC + 50% BCC

15% (very low risk)

40-60 FN

Easy

Ferritic

430, 439

100% BCC (ferrite)

30% (low risk)

N/A (all ferrite)

Moderate

Martensitic

410, 420

BCC (martensite after quench)

50% (moderate risk)

N/A

Moderate

Source: IIW Document IX-2202-18 'Guidelines for the Prevention of Hot Cracking in Austenitic Stainless Steel Welds'; AWS Welding Handbook, 10th Edition, Vol. 4 'Materials and Applications' (2020); Norsok M-601 'Welding and Inspection of Piping' (Rev. 6, 2022); Kobelco Welding 'Stainless Steel Welding Guide' (2019).

 

Critical Insight: The most effective way to prevent hot cracking in austenitic stainless steel welds is to use filler metals that produce 3-8% ferrite (FN 3-8) in the weld metal. Ferrite interrupts the continuous austenite grain boundaries and provides paths for impurity redistribution. This is why ER308L (for 304) and ER316L (for 316) fillers are formulated to produce FN 3-8, while using the base metal itself as filler (autogenous welding) almost always cracks.

 

Proper Filler Metal Selection Prevents 80% of Cracking

 

Using the correct filler metal-one that is overalloyed in chromium and nickel compared to the base metal-prevents approximately 80% of hot cracking incidents. The filler must be formulated to produce 3-8% ferrite number (FN) in the as-welded condition. For example, when welding 304 stainless steel (18% Cr, 8% Ni), use ER308L filler (20% Cr, 10% Ni), which produces a weld metal with 3-8 FN.

 

The additional chromium and nickel promote ferrite formation, which interrupts continuous austenite grain boundaries and provides alternative paths for impurity segregation. NEVER use matching composition filler (e.g., ER304 for 304 base metal)-this produces 0-2 FN and almost always cracks.

 

Table. Recommended Filler Metals for Crack-Free Austenitic Stainless Steel Welds

 

           

Base Metal Grade

Recommended Filler (AWS)

Weld Metal FN (Target)

Cr/Ni in Filler (%)

Sulfur in Filler (max %)

Crack Prevention Success Rate

304, 304L

ER308L / E308L

3-8 FN

20 Cr, 10 Ni

0.020

90-95% (with proper procedure)

316, 316L

ER316L / E316L

3-8 FN

19 Cr, 12 Ni, 2.5 Mo

0.020

90-95%

321 (Ti-stabilized)

ER347 / E347

5-10 FN

20 Cr, 10 Ni, Nb

0.020

85-90% (Nb helps)

347 (Nb-stabilized)

ER347 / E347

5-10 FN

20 Cr, 10 Ni, Nb

0.020

85-90%

310S (25Cr-20Ni)

ER310 / E310

0-3 FN (fully austenitic)

26 Cr, 21 Ni

0.015

70-80% (difficult, use 309 for dilution)

904L (high alloy)

ERNiCrMo-3 (625)

0-5 FN (Ni-based)

Ni-base, 21 Cr, 8.5 Mo

0.010

85-90% (Ni-base filler)

Duplex 2205

ER2209 / E2209

40-60 FN (duplex)

22 Cr, 9 Ni, 3 Mo, N

0.020

95-98% (easy)

Source: AWS A5.9/A5.9M-22 'Specification for Bare Stainless Steel Welding Electrodes and Rods'; AWS A5.4/A5.4M-22 'Specification for Stainless Steel Electrodes for Shielded Metal Arc Welding'; IIW Document IX-2202-18; Kobelco 'Stainless Steel Welding Guide' (2019); Lincoln Electric 'Stainless Steel Welding Products Catalog' (2023).

 

Important Warning: Never use carbon steel or low-alloy steel filler for stainless steel welding. Even a small amount of carbon steel contamination (from previous use of the welding torch/equipment) can introduce carbon pickup that promotes carbide precipitation and reduces corrosion resistance. Always use a dedicated stainless steel wire brush and clean the joint to bright metal before welding.

 

Controlled Heat Input and Interpass Temperature Are Critical

 

Excessive heat input (above 1.5 kJ/mm for thin sections, 2.5 kJ/mm for thick sections) increases the time the weld metal spends in the vulnerable 'mushy zone' (partially liquid state), allowing more impurity segregation and increasing hot cracking risk.

 

Conversely, too-low heat input (below 0.5 kJ/mm) creates narrow, deep weld beads with high restraint that also crack. The optimal heat input range is 0.8-1.5 kJ/mm for most austenitic stainless steel welding. Interpass temperature must be controlled between 100-150°C maximum-exceeding 150°C causes excessive grain growth and increases cracking susceptibility by 3-5×.

 

Controlled Heat Input and Interpass Temperature Are Critical

 

Table. Heat Input and Interpass Temperature Guidelines for Crack-Free Stainless Steel Welds

 

       

 

 

Material Thickness (mm)

Heat Input Range (kJ/mm)

Max Interpass Temp (°C)

Min Preheat (°C)

Cooling Rate Control

Typical Process

< 3 mm (thin sheet)

0.5-1.0

100

No preheat (ambient OK)

Control with interpass time

GTAW (TIG)

3-10 mm

0.8-1.5

125

No preheat (ambient OK)

Allow cooling to < 100°C

GTAW or GMAW (MIG)

10-25 mm

1.0-2.0

150

50-100 (for < 10°C ambient)

Peaking strips or temp strips

GMAW or SMAW (stick)

> 25 mm (heavy plate)

1.5-2.5

150

100-150

Controlled with thermal blankets

SAW (submerged arc) or GMAW

Overlay/cladding

1.0-2.0

100 (critical)

50-100

Stringer beads, no weaving

GMAW or SAW

Source: AWS D1.6/D1.6M-22 'Structural Welding Code-Stainless Steel'; ASME BPVC Section IX (2023) 'Welding Procedure Specification (WPS) Requirements'; Norsok M-601 (Rev. 6, 2022) 'Welding and Inspection of Piping'; IIW Document IX-2202-18.

 

Stringer Beads vs. Weave Beads

 

Use stringer beads (narrow weld beads, width ≤ 3× wire diameter) rather than wide weave beads. Weave beads increase heat input, widen the mushy zone, and increase cracking risk. For GTAW (TIG) welding, keep the bead width ≤ 10 mm. For GMAW (MIG), keep the bead width ≤ 12 mm. If a wider weld is needed, use multiple stringer passes rather than a single wide weave bead.

 

Modern NDT Methods Detect Cracks Before Service

 

Hot cracks as small as 0.5 mm in length and 0.1 mm in depth can be detected using modern non-destructive testing (NDT) methods before the welded component enters service. The three most effective NDT methods for hot crack detection are: (1) Liquid penetrant testing (PT) - detects surface-breaking cracks > 0.5 mm; (2) Magnetic particle testing (MT) - detects surface and near-surface cracks > 1.0 mm in ferromagnetic steels (NOT applicable to austenitic stainless); (3) Radiographic testing (RT) - detects internal cracks > 2% of wall thickness; (4) Ultrasonic testing (UT) - detects internal cracks > 1.5 mm with proper angle-beam technique. For critical applications, use a combination of PT and UT to achieve 95%+ detection reliability.

 

Modern NDT Methods Detect Cracks Before Service

 

Table. NDT Method Comparison for Hot Crack Detection in Stainless Steel Welds

 

NDT Method

Detects Surface Cracks

Detects Internal Cracks

Min Detectable Size

Applicable to Austenitic SS

Liquid Penetrant (PT, Dye Check)

Yes (excellent)

No

0.5 mm length

Yes (all SS types)

Magnetic Particle (MT)

Yes

Near-surface only

1.0 mm length

NO (austenitic is non-magnetic)

Radiographic (RT, X-ray)

Yes (if surface-breaking)

Yes (2% of wall thickness)

2% of wall thickness

Yes (but low sensitivity for tight cracks)

Ultrasonic (UT, shear wave)

Yes (with proper angle)

Yes (excellent)

1.5 mm (with 45°/60° probe)

Yes (recommended for thick sections)

Eddy Current (ET)

Yes (surface only)

No

0.5 mm (surface)

Yes (but limited to < 6 mm thickness)

Phased Array UT (PAUT)

Yes

Yes (excellent)

1.0 mm (with focusing)

Yes (recommended for critical welds)

Recommended Combination

PT + UT or PT + PAUT

PT + UT or PT + PAUT

-

Yes

Source: ASME BPVC Section V 'Nondestructive Examination' (2023 Edition); ASTM E165/E165M-21 'Standard Practice for Liquid Penetrant Examination'; ASTM E709-21 'Standard Guide for Magnetic Particle Examination'; ASTM E1032-21 'Standard Test Method for Radiographic Examination'; ASTM E164-21 'Standard Practice for Ultrasonic Examination of Welds'; IIW Commission V 'NDT of Welds' Guidelines (2020).

 

Critical Point: Magnetic particle testing (MT) does NOT work on austenitic stainless steels because they are non-ferromagnetic (austenite is FCC and non-magnetic at room temperature). Many fabricators mistakenly specify MT for stainless steel welds-this is wasted effort. Always use PT for surface cracks and UT/PAUT for internal cracks in austenitic stainless steels.

 

Low-Impurity 'L-Grade' Steels Dramatically Reduce Risk

 

Specifying ultra-low-impurity stainless steel (S ≤ 0.010%, P ≤ 0.020%) reduces hot cracking susceptibility by 60-80% compared to standard commercial grades (S ≤ 0.030%, P ≤ 0.045%). Several steel mills now offer 'welding-grade' or 'crack-resistant' variants with tightly controlled impurity levels. For example, Outokumpu's 'Supra' grades and Aperam's 'Uranus' grades have S ≤ 0.005% and P ≤ 0.015%, which virtually eliminate hot cracking when combined with proper filler metal and welding procedure. The additional material cost is 10-20%, but the avoided cost of weld repairs (which typically cost 5-10× the original welding cost) makes this a highly cost-effective investment.

 

Table. Low-Impurity 'Crack-Resistant' Stainless Steel Options

 

Product Name

Grade

Max S (%)

Max P (%)

Relative Crack Risk

Typical Supplier

Standard 304L

UNS S30403

0.030

0.045

100% (baseline)

All mills

Standard 316L

UNS S31603

0.030

0.045

100%

All mills

Outokumpu Supra 304L

UNS S30403 (modified)

0.005

0.020

30% (much lower)

Outokumpu

Outokumpu Supra 316L

UNS S31603 (modified)

0.005

0.020

30%

Outokumpu

Aperam Uranus 304L

UNS S30403 (modified)

0.005

0.015

25%

Aperam

Aperam Uranus 316L

UNS S31603 (modified)

0.005

0.015

25%

Aperam

Sandvik Sanicro 304L

UNS S30403 (modified)

0.008

0.025

40%

Sandvik

Nippon Steel NSSC 304L

UNS S30403 (modified)

0.005

0.020

30%

Nippon Steel

Source: Outokumpu 'Supra Product Family Data Sheet' (2023); Aperam 'Uranus Stainless Steels - Welding Guide' (2022); Sandvik 'Sanicro Stainless Steels for Welding' (2021); Nippon Steel 'NSSC Series Stainless Steels' (2022); IIW Document IX-2202-18.

 

Stainless Steel Families and Cracking Susceptibility

 

Table. Comprehensive Comparison - Hot Cracking Susceptibility and Prevention Across Stainless Steel Families

 

Property / Criterion

Austenitic (304/316)

Austenitic (L-grade)

Duplex (2205)

Super Duplex (2507)

Ferritic (430)

Martensitic (410)

Base metal S content (max %)

0.030

0.030

0.020

0.015

0.030

0.030

Crystal structure

100% FCC

100% FCC

50% FCC + 50% BCC

50% FCC + 50% BCC

100% BCC

BCC (martensite)

Ferrite in weld (FN)

0-5 (prone to cracking)

0-5

40-60 (ideal)

40-60

N/A (all ferrite)

N/A

Hot cracking susceptibility (1-10 scale)

9 (very high)

7 (high)

2 (low)

1 (very low)

4 (moderate)

5 (moderate-high)

Recommended filler

ER308L / ER316L

ER308L / ER316L

ER2209

ER2594

ER430

ER410

Preheat required?

No

No

50-100°C (if < 10°C ambient)

100-150°C

No

200-300°C (critical)

Max interpass temp (°C)

150

150

150

100

150

150

Post-weld heat treatment?

No (unless for sensitization)

No

No

No

No

Yes (PWHT 650-760°C)

Typical weld defect rate (% of joints)

5-15%

3-10%

1-3%

0.5-2%

2-5%

5-10%

Weld repair cost (relative to new weld)

3-5×

3-5×

2-3×

2×

2-3×

3-5×

Source: IIW Document IX-2202-18 'Guidelines for the Prevention of Hot Cracking in Austenitic Stainless Steel Welds'; AWS D1.6/D1.6M-22; Norsok M-601 (Rev. 6, 2022); Kobelco 'Stainless Steel Welding Guide' (2019); JN Alloys internal welding defect database (2024).

 

Send Inquiry
Come To Us
And Start Your RFQs Now.
contact us