Quick Answer

 

C-2000 is a strong choice for multi-purpose plants, but it is versatile, not universal. Its 23% chromium helps against oxidizers and ferric ions, its 16% molybdenum against reducing acids and halides, and its 1.6% copper against sulfuric acid. Haynes data show it beating C-276 in sulfuric and nitric acid, yet losing to C-276 in 5% to 20% hydrochloric acid at 66 to 93 °C and in boiling 85% phosphoric acid.

 

Define the exposure envelope before you buy. List every chemical and cleaning agent, the concentration and temperature ranges (including upsets and boiling), contaminants such as oxidizers and halides, crevices, and welds. Screen them against test data, then confirm with a plant coupon test. Also check the code temperature limit: Haynes lists C-2000 to 427 °C, against 677 °C for C-276.

 

Hastelloy C2000 for Multi-Purpose Plants

 

A single-product plant knows what its metal will touch. A multi-purpose plant does not. One week the reactor sees sulfuric acid, the next week hydrochloric acid with a trace of chlorine, then a nitric acid clean. Choosing one alloy for all of it is tempting, and C-2000 is often chosen for exactly that reason.

 

Some suppliers say that with C-2000 you do not need to know exactly what the next batch will contain. The data say otherwise. This article shows how to define the real exposure envelope, where C-2000 leads and trails its neighbors, and what to check before it goes into a vessel. It draws mainly on Haynes International datasheets, ASTM guides, and technical data.

 

What is an exposure envelope, and why does a multi-purpose plant need one?

 

An exposure envelope is the full set of conditions a piece of equipment will see over its life. A multi-purpose plant needs one because the next batch is unknown, so the worst case in every dimension has to be defined, not guessed.

 

A material is only "resistant" inside a set of conditions. Haynes states that its corrosion tables come from reagent-grade acids under laboratory conditions and that field tests are encouraged before industrial use. ASTM G4, the guide for plant coupon tests, adds more reasons for care: dissolved oxygen can change how some alloys behave, high velocity and abrasives are hard to reproduce in coupons, and some materials suffer accelerated corrosion at liquid-to-atmosphere transition zones that small coupons may not cover.

 

Table 1. What goes into an exposure envelope

 

Dimension

What to record

Why it matters

Chemicals

Every process chemical, intermediate, and cleaning agent

Each acid has its own alloy ranking (Table 3)

Concentration

Normal range and extremes, including dilution and evaporation

Rates can change sharply across a concentration band

Temperature

Normal, upset, startup, and boiling conditions

Haynes data show rates jump from the 93 °C column to boiling

Contaminants

Oxidizers (ferric or cupric ions, dissolved oxygen), halides, solids

Oxidizers can ruin alloys built for reducing acids (Section 5)

Local conditions

Crevices, deposits, vapor-liquid lines, dead legs, heat-transfer surfaces

Localized attack starts where a coupon may not look

Metal condition

Welds, cold work, annealing state

Weld metal and cold-worked areas can behave differently (Section 6)

Code limits

Maximum design temperature and pressure class

C-2000's code limit is 427 °C (Section 5)

 

Sources: Haynes International HASTELLOY C-2000 datasheet H-2118C (2023); ASTM G4 (versions 1995 and 2001/2008 via iTeh previews); EETA summary.

 

What does C-2000 add compared with C-276 and C-22?

 

C-2000 adds a deliberate copper addition (about 1.6%) to a high-chromium, high-molybdenum base. That combination is why it is called a "broad-spectrum" alloy, and it is also why its strengths and weak spots differ from C-276 and C-22.

 

Haynes describes C-2000 as unique among the nickel-chromium-molybdenum alloys in having a deliberate copper addition, which greatly enhances sulfuric acid resistance. It also keeps a high chromium level to maximize resistance to oxidizing chemicals and to streams contaminated with ferric ions and dissolved oxygen.

 

Table 2. Composition limits and design intent compared (weight %)

 

Grade (UNS)

Cr

Mo

Cu

Fe

Design idea

C-2000 (N06200)

22.0 – 24.0

15.0 – 17.0

About 1.6 (1.3 – 1.9)

3.0 max

High Cr and Mo plus Cu for sulfuric acid

C-276 (N10276)

14.5 – 16.5

15.0 – 17.0

0.5 max

4.0 – 7.0

Strong in reducing and mildly oxidizing acids

C-22 (N06022)

20.0 – 22.5

12.5 – 14.5

Not added

3.0 – 6.0

Higher Cr for oxidizing media

 

Sources: JN Alloys Hastelloy page (composition table for C276, C22, C2000); Haynes C-2000 and C-276 datasheets for nominal Cu; Zapp Precision Metals C-2000 datasheet for the 1.3 – 1.9% Cu range. Haynes nominal composition for C-2000: Ni 59, Cr 23, Mo 16, Cu 1.6.

 

What this means in practice. Chromium protects against oxidizing attack, molybdenum against reducing attack and halides, and copper against sulfuric acid. A multi-purpose plant that sees both kinds of chemistry, sometimes in the same week, is exactly the use case the alloy was built for. It does not make the chemistry predictable.

 

How does C-2000 compare in the main process acids?

 

C-2000 gives the lowest corrosion rate of the three in sulfuric acid and very dilute hydrochloric acid, while C-276 is lower in 5% to 20% hydrochloric acid at 66 to 93 °C. The ranking depends on the acid, not on the alloy's reputation.

 

How does C-2000 compare in the main process acids

 

Table 3 uses one Haynes laboratory data set that tested C-22, C-276, and C-2000 side by side. Lower numbers are better. The last column shows which of the three had the lowest rate in that row.

 

Table 3. Corrosion rates in mm/y, reagent-grade acids (lower is better)

 

Acid and condition

C-22

C-276

C-2000

Lowest of the three

1% HCl, boiling

0.06

0.33

0.01

C-2000

5% HCl, 93 °C

3.02

1.25

1.37

C-276

5% HCl, boiling

8.90

3.63

4.23

C-276

10% HCl, 79 °C

1.99

1.18

1.54

C-276

20% HCl, 66 °C

0.90

0.55

0.69

C-276

10% H2SO4, boiling

0.29

0.18

0.09

C-2000

30% H2SO4, 93 °C

0.68

0.42

0.04

C-2000

50% H2SO4, 93 °C

0.77

0.62

0.16

C-2000

50% H2SO4, boiling

9.98

3.64

3.35

C-2000 (all high)

70% H2SO4, 93 °C

0.94

0.50

0.42

C-2000

90% H2SO4, 93 °C

1.80

0.46

0.37

C-2000

10% HBr, 93 °C

1.50

0.89

0.34

C-2000

30% HBr, 93 °C

1.12

0.75

0.91

C-276

 

A closer look at hydrochloric acid. Haynes says C-2000 is superior to the other alloys in hydrochloric acid up to 10% on its 0.1 mm/y comparison line. The row data show why that statement needs care. In 10% HCl, C-2000 is lower than C-276 at 38 °C (below 0.01 against 0.17 mm/y) but higher at 66 °C (0.65 against 0.46 mm/y). Once rates exceed about 0.5 mm/y, both alloys are in a range most plants would not accept for long.

 

Table 4. Nitric and phosphoric acid: C-2000 against C-276 (mm/y)

 

Acid and condition

C-276

C-2000

What it shows

40% HNO3, boiling

4.42

0.24

C-2000 far ahead in oxidizing acid

60% HNO3, boiling

18.42

0.94

C-2000 far ahead

70% HNO3, 93 °C

2.62

0.29

C-2000 ahead

50% H3PO4, boiling

0.18

0.03

C-2000 ahead

75% H3PO4, boiling

1.29

0.84

C-2000 slightly ahead

80% H3PO4, boiling

0.31

0.40

About equal

85% H3PO4, boiling

1.68

7.90

C-276 far ahead

 

Sources: Haynes International HASTELLOY C-2000 datasheet H-2118C (2023) and Haynes C-276 datasheet H-2002 (Japanese edition, 2023; haynesintl.com/wp-content/uploads/2024/10/c-276j-1.pdf). Two different datasheets, so treat the comparison as indicative.

 

How do pitting, crevice, and chloride cracking limits compare?

 

C-2000 is very resistant to chloride attack, with a critical crevice temperature higher than C-276. Its critical pitting temperature is slightly lower than C-276's in one Haynes table, and different tests rank the two differently.

 

The ASTM G48 test finds the lowest temperature at which pitting (CPT) or crevice attack (CCT) starts in acidified 6% ferric chloride within 72 hours. Higher is better. Chloride stress corrosion cracking is checked with U-bends in boiling 45% magnesium chloride (ASTM G36).

 

Table 5. Localized corrosion and cracking tests compared (Haynes data)

 

Alloy

CPT in acidified 6% FeCl3

CCT in acidified 6% FeCl3

Boiling 45% MgCl2 (1,008 h)

316L

15 °C

0 °C

Cracked in 2 h

254SMO

60 °C

30 °C

Cracked in 24 h

Alloy 625

100 °C

40 °C

No cracking

C-276

Above 150 °C

55 °C

No cracking

C-2000

145 °C

80 °C

No cracking

 

Source: Haynes International HASTELLOY C-2000 datasheet H-2118C (2023). The HYBRID-BC1 datasheet lists C-2000 CPT as above 140 °C and CCT as 80 °C, consistent within test limits.

 

  • Seawater crevice test (180 days, 29 °C): C-2000 showed no attack in still or flowing seawater, while C-276 had one attacked site per sample in still water (maximum depth 0.10 to 0.13 mm).
  • "Green Death" solution (11.5% H2SO4 + 1.2% HCl + 1% FeCl3 + 1% CuCl2): the lowest temperature at which pitting was seen on C-2000 was 100 °C. For C-276 Haynes reports the boiling point. Here C-276 looks better.
  • "Yellow Death" solution (4% NaCl + 0.1% Fe2(SO4)3 + 0.021 M HCl): no pitting on C-2000 up to 150 °C; critical crevice temperature 95 °C, against 60 °C for C-276. Here C-2000 looks better.

 

Both alloys are far above 316L and 254SMO. Neither is "best" in every test. If chlorides and crevices dominate your envelope, test your own solution.

 

Where does C-2000 not come out ahead?

 

C-2000 trails in hot 5% to 20% hydrochloric acid compared with C-276, in boiling 85% phosphoric acid, in maximum code temperature, and in purely reducing service where a specialist alloy such as B-3 is stronger.

 

Where does C-2000 not come out ahead

 

Table 6. Limits to check in the envelope

 

Condition

What the data show

Alternative to consider

Hot 5% – 20% HCl (66 – 93 °C)

C-276 rates are lower than C-2000 (Table 3); both exceed 0.5 mm/y at higher temperatures

B-3 or HYBRID-BC1 for dedicated, oxidizer-free HCl service

Boiling 85% phosphoric acid

C-2000 at 7.90 mm/y against 1.68 mm/y for C-276 (Table 4)

C-276, after a field test

Code design temperature

C-2000 listed to 800 °F (427 °C); C-276 listed to 1250 °F (677 °C) for ASME VIII-1, B31.3, B16.5, B16.34

C-276 where the design temperature is above 427 °C

Pure reducing acid, no oxidizers

In 5% boiling HCl, B-3 shows 0.08 mm/y against 4.23 for C-2000

B-3, only if oxidizing species are excluded

Oxidizing contamination of a B-type alloy

B-3 corrodes at 47.69 mm/y in acidified 6% FeCl3 at 120 °C, against about 0.5 mm/y for HYBRID-BC1

Keep C-type alloys such as C-2000 where oxidizers may appear

Hydrofluoric acid

Haynes warns HF causes internal as well as external attack of nickel alloys; its tables show external attack only

Field test and inspect; do not rely on the table

 

Sources: Haynes C-2000, C-276, and HYBRID-BC1 datasheets (code tables, uniform corrosion data); EETA summary. Check the current code edition for design limits.

 

Why this matters for the envelope. A multi-purpose plant that chooses C-2000 gains tolerance for the unexpected: Haynes lists its high chromium for streams contaminated with ferric ions and dissolved oxygen. It pays for that tolerance with some loss of peak performance in specific acids. That trade-off is acceptable only if it is made knowingly. A secondary supplier source also notes that C-2000 is generally more expensive than C-276 or C-4; confirm current pricing with your supplier.

 

How do welds and fabrication change the envelope?

 

Weld metal is a different microstructure and can corrode faster or slower than wrought metal, depending on the acid. Anneal after hot forming, and after cold forming of 7% outer-fiber elongation or more.

 

Haynes tested all-weld-metal samples against wrought base metal. Weld metal was higher in sulfuric acid and in 20% hydrochloric acid, but lower in 15% hydrochloric acid, so there is no single rule.

 

Table 7. Weld metal against wrought base metal for C-2000 (mpy)

 

Environment

Weld metal

Wrought base metal

30% H2SO4, 66 °C

0.2

<0.1

70% H2SO4, 66 °C

2.4

0.2

90% H2SO4, 66 °C

2.9

0.6

10% HCl, 38 °C

2.1

<0.1

15% HCl, 38 °C

2.4

7.0

20% HCl, 38 °C

8.0

6.3

30% HNO3, boiling

3.8

3.5

 

Source: Haynes International HASTELLOY C-2000 datasheet H-2118C (2023), "Corrosion Resistance of Welds." Multiply mpy by 0.0254 for mm/y.

 

  • Heat treatment: mill-annealed supply; the annealing temperature is 1149 °C (2100 °F) with water quenching advised (Haynes).
  • Cold work: Haynes says cold work does not usually affect general corrosion or chloride pitting and crevice resistance, but it can affect stress corrosion cracking. Re-anneal after 7% or more outer-fiber elongation.
  • Filler metals: ENiCrMo-17 (electrode) and ERNiCrMo-17 (wire), per the Haynes specification table.
  • Typical hardness: 87 HRBW (sheet), 88 HRBW (plate), 84 HRBW (bar); typical values, not guarantees.

 

How do you build the exposure envelope step by step?

 

List every chemical, set the concentration and temperature ranges including upsets, flag oxidizers and halides, locate the worst spots, screen against published data, and then confirm with a laboratory immersion test and a plant coupon test.

 

Table 8. Step-by-step envelope definition

 

Step

Action

Evidence or tool

1. Inventory

List every process chemical, intermediate, cleaning agent, and rinse. Include planned future campaigns

Process engineering and operations records

2. Ranges

Set concentration and temperature ranges for each, including startup, upset, evaporation, and boiling

Process data; Haynes tables list 93 °C and boiling separately

3. Contaminants

Flag oxidizers (ferric or cupric ions, dissolved oxygen), halides, solids

Haynes notes alloy choice depends on oxidizing contamination (Table 6)

4. Hot spots

Locate crevices, gasket faces, deposits, vapor-liquid lines, dead legs, and welds

ASTM G4 notes transition zones and local factors

5. Screen

Compare each condition with iso-corrosion lines (0.1 and 0.5 mm/y) and the data tables

Haynes datasheets (Tables 3 to 7)

6. Lab test

Run immersion tests in the actual or simulated liquid

ASTM G31 guide

7. Plant test

Expose coupons in the real equipment at representative aeration

ASTM G4 guide

8. Decide

Accept, restrict the campaign list, change alloy, or add inspection

Engineering sign-off

 

Sources: Haynes C-2000 datasheet; ASTM G31 and G4 guides; EETA process. The 0.1 and 0.5 mm/y reading is Haynes' own screening convention in its iso-corrosion diagrams.

 

What plant coupon tests can and cannot show

 

  • They are best at general corrosion. ASTM G4 says tests are designed mainly for general corrosion, and other forms can be assessed with extra examination.
  • Stress corrosion cracking can be invisible. Cracking often causes no significant mass loss, so weight change alone can miss it.
  • Location matters. Coupons should be placed where aeration matches the process, and small coupons may not cover liquid-to-vapor transition zones.
  • One exposure is a snapshot. A single exposure does not show how the rate changes with time.
  • Allow enough time. A commonly cited rule of thumb is at least one week of exposure, with longer being better (secondary summary of G4 guidance).

 

How should the envelope be documented?

 

Use a simple register with one row per chemical or stream, showing ranges, contaminants, evidence, and a decision. A written register stops the next campaign from silently leaving the envelope.

 

How should the envelope be documented

 

Table 9. Example envelope register (illustrative rows built from Haynes laboratory data)

 

Stream

Conditions

Evidence (C-2000, mm/y)

Decision

Sulfuric acid, 30%

93 °C, no halides

0.04 (Haynes table)

Within envelope; confirm with coupons

Sulfuric acid, 70%

93 °C

0.42

Marginal; keep temperature below 93 °C, monitor

Nitric acid, 40%

Boiling

0.24

Within envelope; check weld metal

Hydrochloric acid, 10%

79 °C

1.54

Outside envelope; use a dedicated alloy or lower the temperature

Phosphoric acid, 85%

Boiling

7.90

Outside envelope; use C-276 after a field test

Cleaning agents

To be listed

Not covered by the Haynes tables

Add to register; test before first use

 

What should a buyer write into the purchase order?

 

State the alloy and product standard, the intended envelope or campaign list, the design temperature, the anneal and weld requirements, and the documents to be supplied. A short, written envelope prevents most "it should have worked" disputes.

 

  • Alloy and form: UNS N06200; B575 plate or sheet, B574 bar, B622 or B619/B626 pipe and tube, B366 or B462 fittings, B564 forgings.
  • Condition: solution annealed; state whether the part will be hot- or cold-formed and whether re-annealing is required.
  • Mechanical and composition limits: JN Alloys lists C2000 minimum tensile strength of 690 MPa, yield strength of 310 MPa, and elongation of 45%, with chromium 22.0 to 24.0%, molybdenum 15.0 to 17.0%, iron 3.0% max.
  • Design temperature: state it against the code limit (427 °C for C-2000 in the Haynes code table).
  • Weld consumables: ENiCrMo-17 or ERNiCrMo-17 and a qualified procedure.
  • Sour service: if applicable, name the NACE MR0175 / ISO 15156 edition and condition limits.
  • Documents: EN 10204 3.1 certificate, PMI report (chromium, molybdenum, and copper should match Table 2), and weld records.

 

JN Alloys lists Hastelloy C2000 among its Hastelloy grades in pipes, plates, bars, fittings, forgings, flanges, and prefabricated products. Its published testing equipment includes a spectrum analyzer, universal tensile tester, metallographic analyzer, impact tester, and PMI testing. JN also states that it offers technical consultation to help customers choose materials and processing solutions. Buyers can share their envelope register with JN when requesting a quotation.

 

Frequently Asked Questions

 

Q: What is Hastelloy C2000, and what is its UNS number?

A: Hastelloy C-2000 (UNS N06200, Werkstoff 2.4675) is a nickel-chromium-molybdenum alloy with a deliberate copper addition. Haynes lists nominal 23% chromium, 16% molybdenum, and 1.6% copper. The copper greatly improves sulfuric acid resistance, and the chromium helps with oxidizing chemicals and ferric-ion contamination.

 

Q: Is C-2000 better than C-276?

A: Only in some conditions. In Haynes laboratory data C-2000 has lower corrosion rates in sulfuric acid, nitric acid, and 1% hydrochloric acid. C-276 has lower rates in 5% to 20% hydrochloric acid at 66 to 93 °C and in boiling 85% phosphoric acid. C-2000 also has a lower code temperature limit. The right choice depends on your envelope.

 

Q: What is the maximum code temperature for C-2000?

A: Haynes lists C-2000 for ASME Section VIII Div. 1, B31.3, B16.5, and B16.34 up to 800 °F (427 °C). The same Haynes datasheet for C-276 lists 1250 °F (677 °C) for the same codes. Check the code edition that applies to your equipment.

 

Q: Can one alloy cover every campaign in a multi-purpose plant?

A: No. C-2000 is among the most versatile nickel alloys, but versatile is not universal. A dedicated reducing-acid alloy such as B-3 can beat it in pure hydrochloric acid, while B-3 fails quickly if oxidizing contaminants such as ferric ions are present. The envelope decides, not the alloy's reputation.

 

Q: Does C-2000 resist chloride stress corrosion cracking?

A: Haynes reports no cracking in boiling 45% magnesium chloride (ASTM G36 U-bends) after 1,008 hours, while 316L cracked in 2 hours and 254SMO in 24 hours. Cold work can still affect cracking resistance, so Haynes advises re-annealing parts that had 7% or more outer-fiber elongation.

 

Q: Do laboratory corrosion tables apply directly to my plant?

A: They are a starting point. Haynes states that its tests were done in reagent-grade acids under laboratory conditions and encourages field tests before industrial use. Real streams contain impurities, oxygen, and deposits that change results. ASTM G4 describes how to run coupon tests in plant equipment.

 

Q: What is the typical hardness of C-2000?

A: Haynes reports typical solution-annealed hardness of 87 HRBW for sheet, 88 HRBW for plate, and 84 HRBW for bar. These are typical values, not guaranteed limits. JN Alloys lists minimum tensile strength of 690 MPa, yield strength of 310 MPa, and elongation of 45% for C2000.

 

Q: Which standards cover C-2000 products?

A: Haynes lists ASTM B575 for sheet and plate, B574 for rod and bar, B622 for seamless pipe, B619 and B626 for welded pipe and tube, B366 and B462 for fittings, and B564 for forgings. Weld filler is ENiCrMo-17 (electrode) and ERNiCrMo-17 (wire). It also lists NACE MR0175 / ISO 15156 coverage.

 

Send Inquiry
Come To Us
And Start Your RFQs Now.
contact us