Hastelloy Pump Sleeves: What to Specify for Fit, Finish, and Material Traceability

Nov 24, 2026

Leave a message

Cindy Zhang
Cindy Zhang
Technical Consultant at Jinie Technology, providing expert advice on material selection and processing solutions. Specialized in duplex steel, Hastelloy, and Inconel applications for industrial projects.

Default alloy

Hastelloy C-276 (UNS N10276 / W.Nr. 2.4819), a Ni-Cr-Mo-W alloy with about 15-17% Mo and 14.5-16.5% Cr.

Why a sleeve

A sleeve is a replaceable wear and corrosion barrier. It protects the shaft, housing or stuffing box; it is not the pressure boundary.

Stock form

Machined from ASTM B574 bar or ASTM B564 forging. See Hastelloy C276 product page and technical data sheet.

Fit control

Specify diameter fit, roundness, cylindricity and total runout on the drawing - not just an OD/ID number.

Stock finish guide

Centerless ground bar is typically h9 (about +/-0.02 to 0.05 mm), Ra 0.4-1.6 micrometres; peeled bar is typically h11. Source page

Functional finish

Seal faces Ra 0.8 micrometres or better; bearing journals Ra 0.4-1.6 micrometres. Confirm against the seal vendor.

Traceability

Heat number on the stock before cutting, PMI at receipt, EN 10204 3.1 MTR, and the heat number etched on the finished sleeve.

Machining caution

C-276 work-hardens quickly and holds heat at the edge; keep carbide cutting speeds low and never dwell. Machining guidance

Inspection pack

Dimensional log, MTR, PMI record, surface roughness readings and material marking photograph.

Quality system

JN Alloy manufactures machined parts under an ISO 9001:2015 framework. Certification overview

 

What Does a Hastelloy Pump Sleeve Actually Do?

 

Hastelloy Pump Sleeves

 

A pump sleeve is a replaceable barrier that protects a more expensive shaft, housing or stuffing-box component from corrosion and wear. It is not the pressure boundary, so the specification should focus on fit, surface behaviour and traceability rather than on pressure rating.

 

Think of the sleeve as the sacrificial skin of the pump. In a chemical pump, the sleeve separates the shaft from the pumped acid or chloride solution. In a slurry or marine pump, it takes the rubbing wear at a bearing or packing zone. When the surface is worn or pitted, the sleeve is replaced instead of the shaft. That is why JN Alloy machines sleeves as precision parts: the value is in the geometry and the surface, not in a bulk material certificate alone. See the pump nickel alloy parts range.

 

This distinction changes the purchase. A pressure part is qualified mainly by Code calculations and hydrotest. A sleeve is qualified by whether it drops onto the shaft, runs true, seals cleanly and can be traced back to the exact melt that made it. A buyer who only asks for "Hastelloy" has specified none of those things.

 

Key point: If the sleeve also carries pressure or acts as a retained joint component, say so on the drawing. The inspection and documentation requirements then change, and the supplier must apply the relevant ASME or project rules rather than a general machining route.

 

Why Choose Hastelloy C276 for Pump Sleeves?

 

Choose Hastelloy C-276 when the sleeve sees mixed acids, chlorides or seawater and when ordinary stainless steels pit or stress-corrosion crack. Its molybdenum and tungsten content gives it broad corrosion resistance, while its low carbon and silicon help avoid sensitisation in the weld heat-affected zone.

 

Why Choose Hastelloy C276 for Pump Sleeves

 

C-276 is UNS N10276 / W.Nr. 2.4819. The published composition on the JN Alloy product page lists chromium 14.5-16.5%, molybdenum 15.0-17.0%, tungsten 3.0-4.5%, iron 4.0-7.0%, carbon 0.01% max and silicon 0.08% max. Molybdenum and tungsten resist reducing acids and localised attack; chromium supports the passive film in oxidising conditions. The very low carbon and silicon are why the alloy can be used in the as-welded condition for many services.

 

The technical data sheet gives annealed minimum tensile strength 690 MPa, 0.2% offset yield 283 MPa and elongation 40%. Those numbers are useful for sanity checks, but they are not the reason a sleeve is bought. The reason is that the surface survives the fluid. For a decision framework across corrosive duties, see which alloys suit chemical processing equipment.

 

C-276 is not automatically the right answer. In strongly oxidising media such as hot nitric acid or ferric chloride, C-22 is usually preferred; the difference is explained in C-276 versus C-22. For hot sulfuric acid, other alloys may be more economical. Ask the question "what is the oxidizing or reducing character of the fluid?" before defaulting to C-276.

 

Which Product Form and ASTM Specification Should You Buy?

 

Buy C-276 sleeves from ASTM B574 bar for small, straightforward parts and from ASTM B564 forging when the sleeve is large, heavily stepped or needs a forged grain structure. Both are nickel-alloy specifications; do not substitute ASTM A182, which covers stainless and duplex forgings.

 

The blank route affects cost, lead time and the number of machining setups. Bar is fast and economical for round sleeves. A forging is justified when the part is large, has a flange-like shoulder, or when the customer requires a forged grain flow. JN Alloy explains the difference between open-die and closed-die routes in its forging comparison.

 

Product form and specification map for C-276 pump sleeves

 

Product form

Specification

Use for sleeves

Practical note

Rod and bar

ASTM B574 / ASME SB-574

Small solid sleeves, bushings, wear rings

Most common route; check finish and straightness

Forgings

ASTM B564 / ASME SB-564

Large or stepped sleeves and flanged bodies

Confirm forging route and heat treatment state

Plate

ASTM B575 / ASME SB-575

Flat wear plates and split liners

Not a typical rotating sleeve blank

Seamless pipe and tube

ASTM B622 / ASME SB-622

Long tubular sleeves and liners

Wall tolerance may govern the bore

Welded pipe

ASTM B619 / ASME SB-619

Large-diameter lined sleeves

Weld seam location must be agreed

 

Always write the specification into the purchase order, not just the grade name. The precision nickel alloy parts page shows how JN Alloy routes build-to-print parts from certified stock through finish machining and marking.

 

What Fit Tolerances Should You Specify?

 

Specify fit by function: a bearing journal needs roundness and runout control, a seal face needs flatness and finish, and a press-fit outside diameter needs a defined interference band. A single generic tolerance such as "+/-0.1 mm" is not a fit specification.

 

A sleeve can be dimensionally in tolerance and still fail in service if the bore is out of round or the shoulder is not square to the axis. That is why the drawing should separate size, form and position. For rotating equipment, OD/ID size, concentricity, cylindricity and total runout describe whether the part will run true. Flatness and parallelism describe whether the seal will sit evenly.

 

Functional features to call out on a pump sleeve drawing

 

Feature

What to control

Why it matters

Typical method

Bearing journal OD

Diameter band, roundness, cylindricity, Ra

Controls film thickness and vibration

Fine turn, then grind or polish

Seal face

Flatness, perpendicularity to axis, Ra

Prevents bypass and uneven seal loading

Fine turn or lapping

Shaft bore ID

Diameter band, concentricity to OD

Sets wall uniformity and balance

Finish bore in one setup

Shoulder and groove

Width, depth, squareness, edge break

Locates the sleeve and retains seals

Precision turning with gauges

Thread

Class, pitch diameter, gauge engagement

Prevents cross-threading and loosening

Thread gauge or measuring wire

Wall thickness

Minimum after all machining

Sets corrosion and wear allowance

Ultrasonic or metrology check

 

On precision turned parts, JN Alloy verifies OD, ID, concentricity, cylindricity and total runout during production. The high-precision bearing sleeve and industrial precision liner bushing pages show the category of geometry this applies to. Note that the ISO tolerance class of the incoming bar is a starting point, not the final sleeve tolerance.

 

What Surface Finish Is Right for a Pump Sleeve?

 

Choose surface finish by the job each surface does: a fine, uniform finish on sealing and bearing areas, and a clean but less critical finish elsewhere. Polishing everything is wasteful; leaving a bearing journal as-turned is a common cause of premature wear.

 

What Surface Finish Is Right for a Pump Sleeve

 

The bar finish you start with matters. JN Alloy's round bar finish comparison gives indicative centreless ground tolerance h9 (about +/-0.02 to 0.05 mm) with Ra 0.4-1.6 micrometres, peeled bar h11 with Ra 1.6-3.2 micrometres, and rough turned bar around +/-0.3 to 0.5 mm with Ra 3.2-6.3 micrometres. Centreless ground stock removes less material in the shop and inspects better because the bright surface reveals seams and laps.

 

Indicative surface finish targets by sleeve feature

 

Surface

Indicative Ra target

Reason

Caution

Mechanical seal face

0.4-0.8 micrometres

Low friction and reliable sealing

Confirm with seal supplier

Bearing journal

0.4-1.6 micrometres

Stable lubricant film and low wear

Avoid directional tool marks

Packing area

0.8-1.6 micrometres

Controlled packing bedding

Too smooth can reduce seal life

Non-contact body

1.6-3.2 micrometres

Clean surface at lower cost

Remove all scale and burrs

Weld overlay (if used)

As agreed on drawing

Removes crevice-initiation sites

Inspect for discontinuities

 

Key point: Surface roughness numbers above are indicative workshop and supplier ranges published by JN Alloy, not Code-mandated values. Agree the final Ra with the seal vendor and write it on the drawing. A smoother number is not always better: some packing and elastomer interfaces need a controlled texture to retain lubricant.

 

Nickel alloys rely on a thin passive oxide film. A rough surface gives chlorides more places to concentrate, so a ground or polished finish is often specified for severe corrosion service. The Hastelloy machining guide notes that finishing with CBN is reserved for Ra below 0.8 micrometres, and that white-layer formation must be controlled by speed, coolant and edge condition.

 

How Does Machining Affect Fit and Corrosion Performance?

 

Hastelloy C-276 work-hardens rapidly and conducts heat poorly, so an abusive machining cycle can leave a hardened, stressed surface that changes dimensions and invites corrosion attack. Control heat input, keep the tool cutting and verify surface integrity, not just size.

 

The JN Alloy machining guide reports that C-276 can reach roughly 250-300 HB within the first 0.2-0.5 mm of cut, with locally higher values if the tool rubs. It recommends keeping carbide cutting speeds around 30-60 m/min for turning, using sharp PVD-coated carbide, avoiding dwell and using flood or high-pressure coolant. These are indicative shop ranges, not Code values; the supplier's WPS and machine capability govern.

 

Indicative machining windows for C-276 sleeves (verify in your shop)

 

Operation

Cutting speed

Feed

Depth of cut

Recorded finish

Rough turning

30-50 m/min

0.18-0.25 mm/rev

2.0-4.0 mm

Ra 3.2-6.3 micrometres

Semi-finish turning

40-65 m/min

0.10-0.18 mm/rev

0.75-2.0 mm

Ra 1.6-3.2 micrometres

Finish turning

50-80 m/min

0.05-0.12 mm/rev

0.25-0.75 mm

Ra 0.8-1.6 micrometres

Finish boring

35-70 m/min

0.04-0.08 mm/rev

0.1-0.5 mm

Ra <=0.8 micrometres

Parting / grooving

20-30 m/min

0.03-0.06 mm/rev

2-4 mm blade

Ra 3.2-6.3 micrometres

 

The practical message for a buyer is simple: ask how the supplier protects the finished surface. A supplier who quotes only material cost and cycle time may be grinding through a work-hardened layer and leaving a white layer that is invisible on a dimensional report. Require roughness measurement and, for critical parts, a hardness traverse or surface-integrity check.

 

Key point: Never allow a tool to dwell on a C-276 seal face or journal. A momentary pause can burnish a hard ring that later scores the mating seal. Specify continuous cutting paths and in-process roughness checks on the drawing or quality plan.

 

When Is an Overlay or Hardfaced Sleeve Better Than Solid C276?

 

Use a solid C-276 sleeve when the whole part is small and corrosion exposure is universal. Use a C-276 overlay or weld deposit on a tougher, cheaper substrate when the sleeve is large and only the wetted or rubbing surface needs nickel-alloy performance.

 

Solid material gives the simplest quality case: one heat, one certificate, one material to trace. Overlay lowers material cost and lets the core carry mechanical load, but it adds a bond interface, dilution control and inspection obligations. The decision is economic only when the overlay area and the welding route are defined.

 

If overlay is selected, require the filler metal and welding procedure to be stated. JN Alloy's C-276 filler selection guide discusses ERNiCrMo-4 and the reasons matching filler matters. Control interpass temperature, avoid excessive heat input and define how overlay continuity will be verified. For sour or chloride service, agree any hardness limit with the project specification rather than copying a number from a generic datasheet.

 

Solid C276 versus overlay sleeve - selection summary

 

Criterion

Solid C276 sleeve

C276 overlay on substrate

Selection note

Corrosion barrier

Through the full wall

Wetted surface only

Overlay damage exposes substrate

Traceability

One heat number

Substrate heat plus filler lot

More records to control

Machining risk

Uniform work hardening

Hard overlay over softer core

Tool path must be qualified

Cost driver

Nickel alloy mass

Weld time and inspection

Overlay wins on large parts

Repairability

Limited

Can often be re-overlaid

Agree repair method upfront

 

What Does Material Traceability Have to Prove?

 

Traceability must prove four things: which melt made the sleeve, that the chemistry and mechanical properties match the certificate, that the right material was not mixed with another grade, and that every downstream record points back to the same physical part.

 

A mill certificate is a document about a length of bar. The heat number is the physical link between that document and the piece in your hand. JN Alloy's heat number transfer guide makes the key point clearly: transfer the heat number before the stock enters the cutter. After cutting, the certificate-to-piece relationship has to be reconstructed by length and position, which is an inference rather than a fact.

 

Positive material identification is a separate control. XRF or optical emission confirms the alloy on the component and catches mixed grades in a stores yard. The certificate alone cannot do that. For an overview of how certificates are structured, see understanding steel certificates and how to read a mill test certificate.

 

For fabricated assemblies, the traceability chain must also carry weld numbers, welder identification and filler lots. The traceability discussion explains why records alone are not enough unless the marking on the part agrees with the paperwork. A sleeve may be small, but the audit logic is the same as for a pipe spool.

 

  • Goods receipt: register heat number and certificate number against the physical marking.
  • Receipt PMI: confirm alloy by XRF or optical emission before the material enters production.
  • Before cutting: mark heat number, cut length and part number on the stock.
  • Machining: carry the identity onto the routing card and dimensional log.
  • Marking: laser etch or low-stress mark the finished sleeve; keep tags on the part.
  • Release: check that every heat number in the record exists on a physical item.

 

Which Certificate Level Do You Need: 2.2, 3.1 or 3.2?

 

For most industrial pump sleeves, EN 10204 3.1 is the sensible minimum because it gives certified test values from the mill. Choose 3.2 only when the project or pressure-equipment rules require third-party validation, and 2.2 only for non-critical parts where a declaration is enough.

 

Which Certificate Level Do You Need 22 31 or 32

 

The certificate ladder is often misunderstood. A 2.2 declaration is a statement of compliance without specific test results. A 3.1 certificate gives test results validated by the manufacturer's authorised inspector. A 3.2 certificate adds validation by an independent third party. Buyers who ask for "an MTR" without naming the level leave the supplier to decide.

 

EN 10204 certificate levels applied to pump sleeves

 

Type

Who validates

Typical sleeve use

What to check

2.1

Manufacturer, no test values

Non-critical stock

Not sufficient for a certified sleeve

2.2

Manufacturer declaration

General spares

Statement only; ask for chemistry if needed

3.1

Manufacturer's authorised inspector

Most chemical and marine pump sleeves

Chemistry, mechanical tests, heat number match

3.2

Manufacturer plus independent third party

Pressure equipment or project-specified parts

Third-party stamp and full traceability

 

JN Alloy compares 3.1 and 3.2 in a separate certificate guide. State the required type on the purchase order together with the ASTM product specification, the heat-number marking requirement and the exact records that must accompany the shipment.

 

How Should the Sleeve Be Marked Without Damaging It?

 

Mark the sleeve with a low-stress method such as laser etching, light engraving, etching or a durable tag attached to the part. Deep hard stamping is a poor choice on nickel alloys because the impression can initiate cracking or hide a surface defect.

 

Pump sleeves are often small, curved and later coated or handled roughly, so the marking design matters. JN Alloy's spool marking guidance accepts low-stress stamping, etching, laser marking, indelible ink and durable tags, while warning against deep hard stamping. The same logic applies here.

 

Place the mark on a non-functional band agreed with the designer, never on a seal face or bearing journal.

Use chloride-free and sulfur-free markers where the part will enter high-temperature or corrosive service.

Etch or laser the heat number, part number and batch code so the mark survives handling.

Attach any metal tag to the component, not to the crate; a crate tag identifies packaging, not metal.

Photograph the marking and include the image in the certificate pack.

 

Traceability marking is one of the finishing options listed on the nickel alloy machined parts page, alongside fine turning, grinding, mechanical polishing and chemical passivation. Treat it as part of the process plan, not as a last-minute warehouse task.

 

What Inspection Records Should Ship With Every Sleeve?

 

A complete pack contains the material certificate, PMI record, dimensional log, surface roughness readings, marking photograph and any non-destructive examination report. If the sleeve has an overlay, add the welding and filler-lot records.

 

The purpose of the pack is to let an inspector reconstruct the part without asking the supplier questions. This is exactly the audit logic described in the pipe-spool traceability article: most failures are not missing documents, but two documents that disagree.

 

Recommended release pack for a Hastelloy pump sleeve

 

Record

What it must show

Acceptance check

Mill certificate

EN 10204 3.1 or 3.2, chemistry and mechanical tests

Heat number matches the part mark

PMI report

Alloy confirmation by XRF or OES

Performed on received stock or finished part

Dimensional log

OD, ID, lengths, runout, concentricity, flatness

Each value against drawing tolerance

Surface roughness

Ra at each functional surface

Method and instrument recorded

Marking photograph

Heat number, part number, batch code

Legible and in the agreed zone

NDE / PT report

Surface indication result if required

Referenced to part or batch number

Overlay record

WPS, filler lot, bond inspection

Only for overlay construction

 

What Are the Most Common Specification Mistakes?

 

The recurring mistakes are naming only the alloy, forgetting the certificate level, using one roughness value for every surface, omitting form tolerances, and leaving marking until after the part has been machined and coated.

 

Each mistake is cheap to fix at enquiry stage and expensive after manufacture. A buyer who writes "C276 sleeve, quick quote" will receive a price based on the supplier's assumptions. Those assumptions usually favour the lowest material mass and the shortest machining route, not the longest service life.

 

  1. Writing "Hastelloy" without the UNS number and ASTM product specification.
  2. Assuming C-276 is best in every acid without checking oxidising versus reducing conditions.
  3. Specifying only nominal OD and ID, with no roundness, runout or wall minimum.
  4. Using a single Ra value for seal, journal and body surfaces.
  5. Asking for an MTR without naming EN 10204 3.1 or 3.2.
  6. Allowing the supplier to choose the marking location after machining.
  7. Ignoring work hardening and accepting an unmeasured, as-ground surface.
  8. Buying overlay without defining filler metal, inspection and repair rules.

 

How Do You Compare Suppliers on More Than Price?

 

Compare the evidence, not the alloy name: a supplier who can show a real certificate, a heat-number-to-part link, a dimensional log and a controlled finishing route is quoting a different product from one who cannot.

 

How Do You Compare Suppliers on More Than Price

 

Price differences in machined nickel alloy parts usually come from material yield, machining strategy, inspection depth and documentation. A lower quote may simply mean fewer checks. Ask each bidder to describe the route from certified stock to packed part and request a sample document pack.

 

Supplier evidence checklist

 

Question to ask

Strong answer

Weak answer

Which stock specification?

ASTM B574 or B564 with heat number

"Hastelloy bar"

How is identity preserved?

Mark before cutting, PMI, part-level mark

Certificate kept in a folder

How is finish controlled?

Separate Ra targets and measured values

"CNC finish"

What is in the pack?

MTR, PMI, dimensional log, roughness, photo

Material certificate only

Can you hold form tolerances?

Measured runout and concentricity records

"We can machine it close"

 

JN Alloy's production equipment and certification pages describe the shop and quality framework behind this evidence. Use them as background, but still require project-specific records for your order.

 

What Should a Build-to-Print RFQ Include?

 

A complete RFQ contains the drawing, duty description, alloy and product specification, certificate level, marking rule, inspection pack and quantity with expected annual demand. Without those seven items, price comparisons are meaningless.

 

Send a 2D drawing or 3D model together with the fluid and temperature data. State whether the part is a bearing sleeve, a threaded sleeve or an industrial liner, and link the relevant product family for orientation: bearing sleeve, threaded sleeve, liner bushing. Then add the commercial and quality clauses.

 

Drawing revision and all functional tolerances, including edge breaks.

Fluid composition, chloride level, pH, temperature, pressure and shaft speed.

Alloy UNS number, ASTM product form and condition, for example solution annealed.

EN 10204 certificate type and whether PMI is required.

Surface finish by feature and any passivation or polishing requirement.

Marking method, mark location and photograph requirement.

Inspection pack contents and acceptance criteria.

Quantity, prototype or production status, and required delivery date.

 

How Do You Maintain a Sleeve in Service?

 

Treat the sleeve as a monitored consumable: record installation dimensions, inspect at planned intervals and replace before the wear or corrosion reaches the shaft or housing. Traceability continues after installation because the heat number identifies the material in service.

 

At each shutdown, measure the sleeve at the same locations used in the manufacturing dimensional log. Look for scoring at the seal face, pitting in the wetted zone and any discoloration that suggests temperature excursions. If the pump handles chlorides, pay particular attention to crevice sites under deposits. A sleeve that loses wall thickness locally should be replaced even if the average wear looks acceptable.

 

Keep the certificate pack with the asset record. When a failure is investigated, the ability to trace the sleeve back to a melt and a machining route is what turns an opinion into a diagnosis. That is the practical value of the traceability work described earlier in this guide.

 

Frequently Asked Questions

 

Q1. What is a Hastelloy pump sleeve?

A Hastelloy pump sleeve is a replaceable cylindrical liner, usually machined from Hastelloy C-276 bar or forging, that protects a pump shaft, bearing area or stuffing box from corrosion and wear. It is a wear part, not the pressure boundary. Buy it on fit, finish and traceability.

 

Q2. Why is C-276 the usual alloy for corrosive pump sleeves?

C-276 contains roughly 15-17% molybdenum, 14.5-16.5% chromium and 3-4.5% tungsten, which gives broad resistance to mixed acids, chlorides and localised attack. Its very low carbon and silicon reduce sensitisation, so it is usable in many as-welded conditions.

 

Q3. When should I choose C-22 instead of C-276?

Choose C-22 when the environment is strongly oxidising, for example hot nitric acid or ferric chloride. C-276 remains the stronger choice for reducing acids such as hydrochloric acid. The choice should follow the fluid chemistry, not a generic corrosion chart.

 

Q4. Which ASTM specification covers a C-276 sleeve blank?

Use ASTM B574 or ASME SB-574 for bar and rod, and ASTM B564 or ASME SB-564 for forgings. Do not substitute ASTM A182, which covers stainless and duplex forgings rather than nickel-alloy forgings.

 

Q5. What tolerance matters most on a pump sleeve?

For a rotating sleeve, form control matters as much as size: roundness, cylindricity and total runout determine whether it runs true. Add a defined diameter band, but do not rely on diameter alone.

 

Q6. What surface finish should a mechanical seal face have?

An indicative target is Ra 0.4-0.8 micrometres, but confirm it with the seal supplier. Some packing interfaces need a controlled texture rather than the smoothest possible surface.

 

Q7. Is centreless ground bar necessary for every sleeve?

No. Centreless ground bar, typically h9 with Ra 0.4-1.6 micrometres, suits precision and small-diameter work. Peeled bar at around h11 is more economical for general machining stock. Choose the least expensive finish that meets the next operation.

 

Q8. Why does C-276 work-harden during machining?

C-276 hardens quickly under deformation and conducts heat poorly, so heat stays at the cutting edge. The first 0.2-0.5 mm of cut can reach roughly 250-300 HB. Keep the tool cutting, control speed and coolant, and never dwell.

 

Q9. What cutting speed is typical for C-276 turning?

Indicative shop ranges are 30-50 m/min for rough turning with coated carbide and 50-80 m/min for finishing. Treat these as starting points to be validated in your shop, not Code requirements.

 

Q10. Do I need a certificate with my sleeve?

Yes. For most industrial duties specify EN 10204 3.1, which gives certified test values from the mill. Use 3.2 when a project or pressure-equipment rule requires independent validation.

 

Q11. What is the difference between 3.1 and 3.2 certificates?

A 3.1 certificate is validated by the manufacturer's authorised inspector; a 3.2 certificate is also validated by an independent third party. The extra level adds cost and is justified only when required.

 

Q12. When should the heat number be transferred?

Before the stock enters the cutter. If you mark only after cutting, the link between certificate and piece has to be reconstructed from length and position, which is an inference rather than a fact.

 

Q13. Can I stamp the heat number onto the sleeve?

Use a low-stress method such as laser etching, light engraving or etching on an agreed non-functional band. Deep hard stamping is discouraged on nickel alloys because it can initiate cracking or mask defects.

 

Q14. Should the identification tag be attached to the part or the crate?

To the part. A tag on the crate identifies the packaging, not the component. If the sleeve will be coated or bagged, attach a durable tag that remains visible.

 

Q15. What should a sleeve certificate pack contain?

At least the mill certificate, PMI record, dimensional log, surface roughness readings, marking photograph and any NDE report. Add welding and filler-lot records if the sleeve is overlayed.

 

Q16. Is a solid sleeve better than an overlay sleeve?

Solid C-276 is simpler to trace and inspect and suits small parts. Overlay on a cheaper substrate can be economical for large sleeves, but it adds bond inspection, dilution control and more records.

 

Q17. How do I compare two supplier quotations fairly?

Compare the evidence: stock specification, heat-number control, measured surface finish, dimensional records and certificate pack. A lower price may simply mean fewer inspection steps.

 

Q18. How often should a pump sleeve be inspected in service?

At every planned shutdown, measure the same locations recorded at manufacture and look for pitting, scoring and local wall loss. Replace before damage reaches the shaft or housing, and keep the certificate pack with the asset record.

 